IBS AR-coated SHG/THG LBO crystals for high-power lasers

Frequency conversion of 1064 nm lasers to 532 nm and 355 nm for semiconductor processing, inspection and research

Ultraviolet and green lasers made by frequency-converting 1064 nm Nd:YAG sources are standard tools in semiconductor manufacturing, from wafer marking and via drilling to defect inspection. The nonlinear crystal at the centre of these systems has to survive high peak and average power for years without degrading. This paper explains why lithium triborate (LBO) is the industry's preferred crystal for second-harmonic (SHG, 532 nm) and third-harmonic (THG, 355 nm) generation, compares it with BBO and KTP, and presents the typical parameters of EKSMA Optics LBO crystals with ion beam sputtered (IBS) anti-reflection coatings, including laser-induced damage threshold (LIDT) and absorption measurements at 1064 nm and 355 nm.

1. Frequency conversion with LBO

An Nd:YAG laser emits in the infrared at 1064 nm. Two LBO stages convert it to shorter wavelengths through nonlinear optical effects:

  • Second-harmonic generation (SHG): the 1064 nm fundamental is frequency-doubled in a first LBO crystal to 532 nm (green).
  • Third-harmonic generation (THG): the remaining 1064 nm light is mixed with the 532 nm beam in a second LBO crystal (sum-frequency generation) to produce 355 nm (UV).

Both processes rely on the second-order nonlinear susceptibility, χ(2), of the crystal.[1] At high optical intensity, the polarisation induced in the crystal contains a component that oscillates at twice the input frequency, or at the sum of two input frequencies. Energy is conserved photon by photon: two 1064 nm photons combine into one 532 nm photon, and a 1064 nm photon plus a 532 nm photon combine into one 355 nm photon (1/1064 + 1/532 = 3/1064, i.e. 354.7 nm). At low conversion the generated power grows roughly with the square of the input intensity, so efficient harmonic generation needs high peak power. This is why most of these systems use Q-switched nanosecond or mode-locked picosecond lasers.

Conversion only builds up along the crystal if the input and generated waves stay in phase. Because of normal dispersion, the refractive index is higher at shorter wavelengths, so in an isotropic material the harmonic would drift out of phase with the fundamental within tens of micrometres. LBO is birefringent. Choosing the propagation direction and polarisations so that the fundamental and the harmonic see the same refractive index brings the phase mismatch, Δk, to zero. In Type I phase matching both input photons have the same polarisation; in Type II they are orthogonally polarised.

There are two ways to reach this condition. In critical phase matching (CPM) the crystal is cut at an angle to its optical axes. This works at room temperature, but the generated beam walks off from the fundamental and the angular acceptance is narrow. In non-critical phase matching (NCPM) the beam travels along a principal axis of the crystal and the crystal is temperature-tuned instead; for 1064 nm SHG, Type I NCPM is reached in LBO at about 149 °C.[2] Walk-off then disappears and the angular acceptance becomes very wide, so longer crystals and tightly focused or less-than-ideal beams can be used. SHG crystals are therefore usually held in a temperature-stabilised oven. For THG, LBO is normally used in critical phase matching, in either Type I or Type II.

The two stages also have to be balanced. Sum-frequency generation works best when the 1064 nm and 532 nm beams entering the THG crystal carry equal numbers of photons, which corresponds to converting about two-thirds of the fundamental power to green in the first stage. The polarisations must suit the phase-matching type of the THG crystal, so a dual-wavelength waveplate is often placed between the stages, and the two beams must overlap in space and time inside the second crystal.

Each stage shortens the wavelength, and each LBO crystal and its coated surfaces must carry the full power of the beam passing through it. Crystal and coating quality therefore set the power, efficiency and lifetime of the whole laser.

2. Applications

Frequency-converted Nd:YAG and Nd:YVO4 lasers are the workhorse sources of the semiconductor industry because they combine short wavelength with the pulse energy, repetition rate and reliability that production lines require. Green (532 nm) and ultraviolet (355 nm) light are absorbed strongly by silicon, metals, polymers and many compound semiconductors, can be focused to a spot a few micrometres across, and deposit their energy in a thin surface layer. The sections below outline where these sources are used, and what each use demands of the LBO crystals inside them.

2.1 UV laser sources for semiconductor micromachining

Short-wavelength light couples into material at the surface with little heat spread, which is why 355 nm sources produced by LBO THG are used across wafer processing:

  • Wafer marking and serialisation. UV lasers engrave serial numbers, lot codes and data-matrix barcodes onto silicon wafers. Because the light is absorbed at the surface with minimal heat, marks are clean and the wafer is not damaged.
  • Via drilling and scribing. Frequency-converted UV lasers drill microvias, the small interconnect holes between chip layers, and scribe or dice wafers into individual dies. LBO enables the high-power, short-wavelength beams needed for clean, debris-free cuts in silicon, GaN and SiC.
  • Laser lift-off at 355 nm. UV pulses fired through the sapphire decompose a thin layer of GaN at the interface and release the GaN epilayer from the substrate. The process was demonstrated with the 355 nm third harmonic of a Q-switched Nd:YAG laser[12] and with a 248 nm KrF excimer laser.[3] It is a critical step in manufacturing micro-LEDs and vertical LEDs, where the GaN layer is transferred onto a different carrier substrate for packaging.

Micromachining sources are typically diode-pumped solid-state lasers with nanosecond pulses of 10–30 ns at repetition rates from tens to hundreds of kilohertz and UV average powers from a few watts to several tens of watts. For glass, sapphire and SiC, picosecond versions of the same architecture are used, where the much higher peak intensity makes cold ablation possible but also places the harshest demands on the crystal. These lasers run around the clock in fabs, so the SHG and THG stages must deliver stable output over many thousands of hours. UV output is where lifetime is usually lost: any absorption in the THG crystal or its coatings heats the crystal, shifts the phase-matching condition and lowers the conversion efficiency, while surface contamination or coating damage ends the life of the component altogether.

2.2 UV laser sources for wafer and photomask inspection

  • Wafer surface inspection. Light scattering from defects depends on wavelength, so shorter wavelengths detect smaller defects. 355 nm UV light finds yield-critical particles, scratches and voids that visible 532 nm light can no longer resolve, and at the most advanced nodes inspection moves further into the deep UV, to 266 nm and shorter.
  • Photomask and reticle inspection. UV imaging resolves nanoscale defects on photomasks. A single missed mask defect is reproduced on every wafer the mask prints and can cause millions of dollars of waste.

Inspection sources have different priorities from machining sources. They operate at very high repetition rates or quasi-continuously, at moderate power, and the critical parameters are low intensity noise, high beam-pointing stability and a long, predictable service interval, because a drifting source produces false defect counts and tool downtime. For the frequency-conversion stage this translates into a demand for highly homogeneous crystals with very low bulk and surface absorption, so that the thermal lens and the phase-matching temperature stay constant as the laser runs. The low absorption and scatter of IBS-coated LBO, demonstrated in Section 6, are directly relevant here.

2.3 Other application areas

Outside the semiconductor sector, the same 532 nm and 355 nm sources are used wherever a short wavelength, a high beam quality and reliable high power are needed. Table 1 groups the main application areas.

Green sources deserve a separate mention. The 532 nm output of an LBO SHG stage is the standard pump for Ti:sapphire oscillators and amplifiers in research laboratories, and in industry it is increasingly used for welding and cutting copper, which absorbs green light several times more strongly than infrared,[4] for example in battery and electric-motor manufacturing. Across all of these areas the demands on the crystal are the same as in semiconductor processing: high conversion efficiency, a damage threshold well above the operating fluence, and output that stays stable over years of service.

AreaTypical uses
Industrial UV laser generationMicromachining of glass, polymers and semiconductors; PCB drilling and structuring; high-precision material processing
High-power green generationPump sources for Ti:Sapphire lasers; materials processing; scientific and industrial laser systems
Scientific and researchSpectroscopy and nonlinear optics experiments; frequency conversion in tunable laser systems; B-integral correction in the low-power regime
Medical and bio-photonicsUV sources for imaging and diagnostics; precision laser surgery systems; skin care at 532 nm

Table 1. Typical uses of LBO-based SHG and THG sources.

3. Why the industry chooses LBO

Four material properties make LBO the default crystal for high-power SHG and THG:

  • High damage threshold: the crystal handles high-power lasers reliably.
  • Broad transparency range: it works across applications from the UV to the IR.
  • Thermal and mechanical stability: performance stays consistent under thermal and mechanical stress.
  • Non-critical phase matching (NCPM): non-critical phase matching lowers system complexity and gives the best conversion to the second harmonic.

Lithium triborate, LiB3O5, is a biaxial crystal of the orthorhombic mm2 point group, grown from a high-temperature flux solution.[5] It is transparent from about 160 nm in the vacuum ultraviolet to about 2.6 µm in the infrared, so it passes the fundamental, the second harmonic and the third harmonic with negligible intrinsic absorption. Its effective nonlinear coefficient is moderate, lower than that of BBO or KTP, but this is more than compensated in practice: the very high damage threshold allows the crystal to be driven at higher intensity, the wide angular acceptance and small walk-off allow long crystals to be used, and the availability of non-critical phase matching removes walk-off altogether for SHG. LBO is also only slightly hygroscopic, and with a Mohs hardness of 6 it takes a durable, high-quality polish that is a good base for coatings.

Table 2 compares LBO with the two other common choices for 1064 nm SHG, BBO and KTP. LBO's bulk damage threshold is roughly 3.5 times that of BBO, and it is the only one of the three rated excellent for power scaling.

PropertyLBOBBOKTP
Laser damage threshold (bulk)~177 J/cm² (10 ns, 10 Hz)~50 J/cm² (10 ns, 10 Hz)Depends strongly on growth method
Operational stabilityHighModerateModerate
Walk-off angle7 mrad56 mrad4 mrad
Angular acceptance6.5 mrad·cm0.58 mrad·cm9.42 mrad·cm
Power scaling capabilityExcellentVery limitedModerate
Mohs hardness645

Table 2. LBO compared with BBO and KTP for SHG at 1064 nm.

Sources: references [9]–[11] and the EKSMA Optics catalogue. Walk-off and angular acceptance refer to SHG of 1064 nm in critical phase matching (Type I for LBO and BBO, Type II for KTP).

The comparison explains the choice. BBO has a higher nonlinearity, but its large walk-off angle of 56 mrad and narrow angular acceptance limit the usable crystal length and beam quality, it is hygroscopic, and its lower damage threshold restricts power scaling. KTP offers the highest nonlinearity and the smallest walk-off, but at high green power it suffers from grey tracking, a gradual photo-induced darkening that raises absorption and destabilises the output,[6] and its damage threshold varies strongly between growth methods. LBO has none of these failure modes, which is why it dominates in industrial SHG and THG stages running at tens of watts and above. BBO remains the better choice for fourth-harmonic generation at 266 nm and for very short pulses, where its higher nonlinearity and deeper UV phase-matching range are needed.

4. Typical SHG and THG parameters

Tables 3 and 4 list typical design parameters for LBO in the two conversion stages.

The values are indicative. The exact phase-matching angle or temperature, the acceptance bandwidths and the achievable efficiency depend on the fundamental wavelength, the pulse duration, the beam quality and the crystal length, and EKSMA Optics calculates and cuts each crystal for the customer's specific operating point.

ParameterTypical value
Fundamental wavelength range551–2600 nm (Type I phase matching)
Phase matchingType I (often non-critical)
Effective nonlinearity (deff)~0.8–1 pm/V (Type I, 1064 nm)
Walk-off angle0 (NCPM); ~7 mrad (CPM)
Temperature bandwidth~4 °C·cm FWHM (NCPM)

Table 3. Typical LBO parameters for SHG.

For SHG of 1064 nm the usual choice is Type I non-critical phase matching along the crystal's x axis at about 149 °C, with the crystal held in a small oven. Because walk-off is zero, the crystal can be made as long as the temperature bandwidth allows: with a bandwidth of roughly 4 °C·cm (FWHM), a 20 mm crystal has a bandwidth of about 2 °C. A standard oven controller holds the crystal to ±0.1 °C, a small fraction of this window, so the temperature requirement is easily met even for 30 mm crystals and leaves margin for the slight heating caused by absorbed laser power. Where an oven is not wanted, Type I critical phase matching at room temperature is used instead, at the cost of about 7 mrad of walk-off that limits the useful length to around 10–20 mm for a typical beam size. Typical SHG crystals have apertures of 3 × 3 mm to 10 × 10 mm and lengths of 10–30 mm, and in nanosecond systems they convert well over half of the fundamental power to green.

ParameterTypical value
Process1) SHG 1064 → 532 nm; 2) SFG 1064 + 532 → 355 nm
Phase matchingType I / Type II
Angular sensitivity~1.2 mrad FWHM (20 mm crystal)
SHG stage efficiency>60% (1064 → 532 nm, pulsed, 10 ns)
Overall THG efficiency~30–40% (1064 → 355 nm, ns pulsed)
Temperature acceptance~1.4 K
Output power stability≤1.3% RMS

Table 4. Typical LBO parameters for THG.

The THG stage is more demanding. Sum-frequency mixing of 1064 nm and 532 nm in LBO uses critical phase matching, so the crystal is cut at an angle and both walk-off and the angular acceptance have to be managed. An angular sensitivity of about 1.2 mrad FWHM for a 20 mm crystal means the mount must be stable to a fraction of a milliradian and the beams must have a divergence well below that figure, which usually sets the crystal length at 10–20 mm. The temperature acceptance of about 1.4 K is wide enough for room-temperature operation with a thermoelectrically stabilised mount. The main practical limit is thermal: the small residual absorption of the crystal and its coatings at 355 nm heats the crystal, shifts it off phase matching and can create a thermal lens, so the UV output of a high-power laser is only as stable as the absorption of its THG crystal is low. This is the reason the absorption measurements in Section 6 matter as much as the damage threshold.

5. Ion beam sputtered AR coatings

A crystal's performance is limited by its surfaces as much as its bulk. EKSMA Optics coats its SHG and THG LBO crystals using ion beam sputtering (IBS), which produces dense, low-loss anti-reflection layers. IBS coatings offer:

  • Low scatter at SHG and THG wavelengths
  • High damage threshold
  • Improved long-term reliability
  • Excellent spectral performance
  • Suitability for high peak and high average power

In ion beam sputtering, a broad beam of argon ions from an ion source strikes a target of the coating material inside a high-vacuum chamber (Figure 1). Atoms sputtered from the target arrive at the substrate with kinetic energies of several electronvolts, an order of magnitude higher than in thermal or electron-beam evaporation,[7] and pack into dense, amorphous layers with practically no voids. Layer thickness is controlled by in-situ optical monitoring, so the finished stack lands on its design wavelengths without the moisture-induced spectral shift that porous evaporated films show when they leave the chamber. The result is a coating with very low scatter and absorption, a damage threshold close to that of the bare substrate, and spectral performance that does not drift with humidity or temperature.

Anti-reflection coatings for LBO have to meet unusual requirements. Each crystal face sees more than one wavelength: the SHG crystal needs low reflectance at 1064 nm and 532 nm on both faces, and the THG crystal's output face must handle 1064, 532 and 355 nm at once. LBO's low refractive index of about 1.6 leaves little room for a simple single-layer design, so multilayer stacks of oxides are used, with low-absorption materials selected for the UV. LBO also expands anisotropically with temperature, and SHG crystals are cycled daily between room temperature and about 150 °C, so the coating must be designed and deposited to withstand this stress without crazing or delamination. The dense, well-adhered layers produced by IBS are well suited to this.

Ion beam sputtering chamber, side view. An ion source on the left wall fires a straight beam of argon ions at a tilted sputter target, and a neutralizer on the floor next to the source feeds electrons into the beam. Atoms knocked out of the target travel up in a widening plume to a rotating substrate holder at the top and coat the downward-facing substrates. An assist ion source mounted through the chamber floor points a second, weaker ion beam from the middle of the floor that widens symmetrically to cover the whole substrate holder. A witness piece sits on the same holder near its centre, and an optical monitor above the chamber measures it through windows in the lid and the holder as the layers grow. In-situ optical monitor Assist ion source e− Neutralizer Ion source Ion beam Substrate holderrotating Substrates Sputtered atomsseveral eV Witness piece Sputter target High-vacuumchamber
Figure 1. Schematic of an ion beam sputtering deposition chamber.
ParameterTypical valueCondition
Common wavelengths1064 / 532 / 355 nmSHG / THG
Reflectivity (AR)R < 0.1%Per surface
Absorption< 10 ppmAt 1064 nm
Scatter loss< 10 ppmAt 1064 nm
Damage threshold> 80 J/cm²10 ns, 1064 nm

Table 5. Typical IBS AR coating parameters.

Every coating run is verified by spectrophotometry, and samples are tested for absorption by photothermal methods and for damage threshold according to ISO 21254, as described in the next section.

6. Measured damage threshold and absorption

Two measurements characterize how a coated crystal will behave at high power. The laser-induced damage threshold (LIDT) was measured in an S-on-1 test according to ISO 21254: a grid of sites on the coated surface is exposed to a fixed number of pulses at increasing fluence, with online scatter detection to register the first sign of damage and microscope inspection afterwards. Plotting the highest fluence survived against the number of pulses, from 10 to 1000, shows whether the surface fatigues under repeated exposure, which is what matters in a laser running at kilohertz repetition rates for years. Absorption was measured by a photothermal technique in which a modulated pump beam heats the sample and a probe beam senses the resulting refractive-index change, giving absorption in parts per million with a spatial resolution that separates the two coated faces from the bulk.[8]

6.1 At 1064 nm

Figure 2 shows the damage curve of a coated LBO sample tested at 1064 nm with (9.9 ± 0.3) ns pulses at 100 Hz, 0° angle of incidence, linear polarization and a (238.3 ± 4.2) µm beam diameter (1/e²). The highest fluence before first damage stays near 100 J/cm² from 10 to 1000 pulses, so the threshold does not fall with repeated exposure. Figure 3 shows a longitudinal absorption scan of a sample at 1070 nm (2.0° AOI, linear P polarization): absorption peaks at the two crystal faces and stays low through the bulk.

Laser-induced damage threshold of sample LBO_Stand_1 at 1064 nm, 9.9 ns pulses, 100 Hz: about 98 J/cm² at 10, 100 and 1000 pulses, with a 95% confidence band from about 83 to 113 J/cm².020406080100120140160180200Fluence, J/cm²101102103Number of pulsesOffline detectionOnline detection95% confidence intervalSample name:LBO_Stand_1Wavelength:1064 nmPulse duration:(9.9 ± 0.3) ns FWHMRepetition rate:100 HzAOI:0 degPolarization:LinearBeam diameter:(238.3 ± 4.2) µm, 1/e²
Figure 2. LIDT at 1064 nm: highest threshold before first damage versus number of pulses.

These results leave a wide safety margin. A nanosecond SHG stage typically operates at a fluence of a few J/cm² on the crystal, so a threshold near 100 J/cm² corresponds to a margin of more than an order of magnitude. The flat damage curve between 10 and 1000 pulses shows no incubation effect, that is, repeated exposure below threshold does not weaken the surface. The absorption scan confirms that the bulk crystal contributes very little heating and that the remaining absorption sits at the surfaces, within the coating and the polished layer beneath it, which is exactly where the IBS process gives the most control.

Absorption signal along an 11 mm path at 1070 nm: peaks of about 6 to 7 ppm at the two crystal surfaces, near -10 mm and 0 mm, and a low flat signal through the bulk in between. The right-hand scale gives the same signal in bulk units, ppm/cm.0246810Surface absorption, ppm050100150200250300350Bulk absorption, ppm/cm−10−8−6−4−20Distance, mmSample name:KRI9485-191382-2Wavelength:1070 nmAOI:2.0 degPolarization:Linear PProtocol:L scanLocation:Front surface
Figure 3. Longitudinal absorption scan at 1070 nm (surface and bulk absorption versus position).

6.2 At 355 nm

Figure 4 shows the characteristic damage curve at 355 nm with (5.5 ± 0.3) ns pulses at 100 Hz, 0° AOI, linear polarisation and a (219.1 ± 3.8) µm beam diameter. With online detection the threshold stays near 20 J/cm² from 10 to 1000 pulses.

A lower threshold at 355 nm is expected:[9] the photon energy is three times higher, the pulses are shorter, and both crystal and coating materials absorb more in the UV. Even so, a threshold near 20 J/cm² (the dot at 5 J/cm² was a defect) sits well above the fluence of roughly 1–2 J/cm² at which a THG crystal is normally run, and the curve is again flat from 10 to 1000 pulses. The absorption scan at 355 nm tells the same story as at 1064 nm: the faces dominate, the bulk is clean. For a UV laser this is the critical result, because surface absorption is what drives the slow heating and efficiency drift that limits the lifetime of THG stages, and it is the quantity that polishing and coating quality can improve.

Damage of IBS anti-reflection coatings on LBO has been studied in detail in Vilnius. Abromavičius et al. measured the multi-pulse LIDT of single-wavelength (AR@355 nm) and triple-wavelength (AR@355+532+1064 nm) coatings at 355 nm and found designs based on ZrO2–SiO2 mixtures generally more damage-resistant than conventional Al2O3/SiO2 stacks.[13] Atkočaitis et al. later showed that the multi-pulse LIDT of such coatings scales approximately as τ0.5 with pulse duration τ across the picosecond-to-nanosecond range.[14] This scaling allows the results above to be compared with other suppliers' data, which are usually quoted for 10 ns pulses. The 1064 nm test, at 9.9 ns, needs no correction; the 355 nm threshold measured with 5.5 ns pulses corresponds to roughly 27 J/cm² at 10 ns.

Laser-induced damage threshold of sample KRI9915-209556-355 at 355 nm, 5.5 ns pulses, 100 Hz: with online detection about 20 J/cm² at 10, 100 and 1000 pulses; a single offline-detection point at about 5 J/cm² at 1000 pulses.05101520253035Fluence, J/cm²101102103Number of pulsesOffline detectionOnline detection95% confidence intervalSample name:KRI9915-209556-355Wavelength:355 nmPulse duration:(5.5 ± 0.3) ns FWHMRepetition rate:100 HzAOI:0.0 degPolarization:LinearBeam diameter:(219.1 ± 3.8) µm, 1/e²
Figure 4. LIDT at 355 nm: characteristic damage curve versus number of pulses.

7. Key strengths of EKSMA Optics LBO crystals

StrengthWhat it means in a laser system
High optical qualityLow bulk absorption and scatter; very high homogeneity for stable beam propagation
High damage thresholdOptimised for high peak and high average power; suited to demanding SHG and THG applications
IBS coatingsLow-loss, high-LIDT coatings with consistent performance across 1064 / 532 / 355 nm
Thermal and mechanical reliabilityStable operation under high thermal load; proven long-term performance in industrial systems

Table 6. Summary of EKSMA Optics IBS AR-coated LBO crystals.

Conclusion

Semiconductor marking, drilling, lift-off and inspection all depend on stable 532 nm and 355 nm sources, and those sources are only as reliable as their nonlinear crystals. LBO combines a bulk damage threshold several times higher than BBO with good power scaling and thermal stability, and IBS anti-reflection coatings bring surface losses below 0.1% reflectance and 10 ppm absorption at 1064 nm. Together they give laser manufacturers a frequency-conversion stage built for high power and long service life.

Tell us your SHG/THG crystal spec

Discuss your project with one of our sales engineers.

LBO SHG/THG crystal FAQ

  • Why is LBO preferred over BBO and KTP for high-power SHG and THG?

    LBO's bulk damage threshold is roughly 3.5 times that of BBO, and it is the only one of the three rated excellent for power scaling. BBO's large walk-off angle of 56 mrad and narrow angular acceptance limit the usable crystal length and beam quality, and KTP suffers from grey tracking at high green power. LBO has none of these failure modes, which is why it dominates in industrial SHG and THG stages running at tens of watts and above.

  • At what temperature is LBO non-critically phase matched for 1064 nm SHG?

    For SHG of 1064 nm the usual choice is Type I non-critical phase matching along the crystal's x axis at about 149 °C, with the crystal held in a small oven. Because walk-off is zero, the crystal can be made as long as the temperature bandwidth allows: with a bandwidth of roughly 4 °C·cm (FWHM), a 20 mm crystal has a bandwidth of about 2 °C.

  • Why use ion beam sputtered AR coatings on LBO?

    Atoms sputtered from the target arrive at the substrate with kinetic energies of several electronvolts and pack into dense, amorphous layers with practically no voids. The result is a coating with very low scatter and absorption, a damage threshold close to that of the bare substrate, and spectral performance that does not drift with humidity or temperature.

  • What damage threshold do IBS-coated LBO crystals reach?

    At 1064 nm the highest fluence before first damage stays near 100 J/cm² from 10 to 1000 pulses. At 355 nm, with 5.5 ns pulses, the threshold stays near 20 J/cm², which corresponds to roughly 27 J/cm² at 10 ns. Both sit well above the fluences at which SHG and THG crystals are normally run.

References

  1. R. W. Boyd, “The nonlinear optical susceptibility”, in Nonlinear Optics, 3rd ed. Burlington, MA: Academic Press, 2008, pp. 1–67, doi: 10.1016/B978-0-12-369470-6.00001-0.
  2. T. Ukachi, R. J. Lane, W. R. Bosenberg, and C. L. Tang, “Measurements of noncritically phase-matched second-harmonic generation in a LiB3O5 crystal”, Appl. Phys. Lett., vol. 57, no. 10, pp. 980–982, Sep. 1990, doi: 10.1063/1.104275.
  3. W. S. Wong, T. Sands, and N. W. Cheung, “Damage-free separation of GaN thin films from sapphire substrates”, Appl. Phys. Lett., vol. 72, no. 5, pp. 599–601, Feb. 1998, doi: 10.1063/1.120816.
  4. S. Engler, R. Ramsayer, and R. Poprawe, “Process studies on laser welding of copper with brilliant green and infrared lasers”, Phys. Procedia, vol. 12, pp. 339–346, 2011, doi: 10.1016/j.phpro.2011.03.142.
  5. C. Chen et al., “New nonlinear-optical crystal: LiB3O5”, J. Opt. Soc. Am. B, vol. 6, no. 4, pp. 616–621, Apr. 1989, doi: 10.1364/JOSAB.6.000616.
  6. B. Boulanger, M. M. Fejer, R. Blachman, and P. F. Bordui, “Study of KTiOPO4 gray-tracking at 1064, 532, and 355 nm”, Appl. Phys. Lett., vol. 65, no. 19, pp. 2401–2403, Nov. 1994, doi: 10.1063/1.112688.
  7. D. T. Wei, “Ion beam interference coating for ultralow optical loss”, Appl. Opt., vol. 28, no. 14, pp. 2813–2816, Jul. 1989, doi: 10.1364/AO.28.002813.
  8. M. Commandré and P. Roche, “Characterization of optical coatings by photothermal deflection”, Appl. Opt., vol. 35, no. 25, pp. 5021–5034, Sep. 1996, doi: 10.1364/AO.35.005021.
  9. F. R. Wagner, A. Hildenbrand, J.-Y. Natoli, and M. Commandré, “Nanosecond-laser induced damage at 1064 nm, 532 nm, and 355 nm in LiB3O5”, presented at Laser Damage Symposium XLI: Annual Symposium on Optical Materials for High Power Lasers, G. J. Exarhos, V. E. Gruzdev, D. Ristau, M. J. Soileau, and C. J. Stolz, Eds., Boulder, CO, Oct. 2009, paper 75041M, doi: 10.1117/12.836489.
  10. C. Zhang et al., “Growth of KTP crystals with high damage threshold by hydrothermal method”, J. Cryst. Growth, vol. 292, no. 2, pp. 364–367, Jul. 2006, doi: 10.1016/j.jcrysgro.2006.04.036.
  11. V. G. Dmitriev, G. G. Gurzadyan, and D. N. Nikogosyan, Handbook of Nonlinear Optical Crystals, 3rd ed., Springer Series in Optical Sciences, vol. 64. Berlin, Germany: Springer, 1999; and SNLO software, AS-Photonics.
  12. M. K. Kelly, O. Ambacher, R. Dimitrov, R. Handschuh, and M. Stutzmann, “Optical process for liftoff of group III-nitride films”, Phys. Status Solidi A, vol. 159, no. 1, pp. R3–R4, Jan. 1997, doi: 10.1002/1521-396X(199701)159:1<R3::AID-PSSA99993>3.0.CO;2-F.
  13. G. Abromavičius et al., “Optical resistance and spectral properties of anti-reflective coatings deposited on LBO crystals by ion beam sputtering”, Lith. J. Phys., vol. 51, no. 4, pp. 303–308, 2011, doi: 10.3952/lithjphys.51407.
  14. E. Atkočaitis, L. Smalakys, and A. Melninkaitis, “Pulse temporal scaling of LIDT for anti-reflective coatings deposited on lithium triborate crystals”, Opt. Express, vol. 30, no. 16, pp. 28401–28413, Aug. 2022, doi: 10.1364/OE.459391.